Stuck Shot

Description

Defect Type

Positive

Appearance

Smooth - round, oval, or hemispherical

Size

1/8” or less

Typical Location

Highly detailed areas such as depressed lettering or score lines

Similar to
Aliases

Positive metal

Method for defect determination

Stuck shot can be pried out. Can also section, mount and polish through defect. Stuck shot will not be attached to the casting – only wedged in place

Mechanism

Shot wedged into lettering or detailed areas during shot blasting operation

Corrections

Other (Shot blast) Shot is the wrong size for the part

Change the shot size